·After the ITO is patterned the ACTFEL lamp can
made.
·Each layer comes packaged separately as a thick paste
(stir before using).
·The thickness of each layer is controlled by using
scotch tape as a spacer.
·Apply scotch tape along 3-5mm on two parallel sides of
the plate.
·Apply the pastes in sequence using a spatula. Thin
them by scraping a microscope slide across
the layer.
·Dry and cure each layer before application of the next
-Each layer is dried in an oven at 130°C for ~15 minutes.
·1st phosphor (Luxprint 8152)
·2nd dielectric (Luxprint 8153)
·3rd conductive silver rear electrode
(Luxprint 9145)